Monocrystalline alloy with a nickel base matrix
Ключевые слова
Патентная информация
Номер патента | 4818306 |
Подан | 02/23/1986 |
Дата патента | 04/03/1989 |
абстрактный
Претензии
What is claimed is:
1. Monocrystalline alloys with a nickel base matrix, without intentional addition of carbon, of boron or of zirconium, consisting essentially of a composition by weight as follows:
with, in addition, a summation of atomic percentages: 0.005Co+0.036Cr+0.052Mo+0.066W+0.026Al+0.116Nb+0.049Ta less than or equal to one, and a summation of atomic percentages: Ta+W+Mo+Nb between 5.9 and 6.3, the alloys being free of titanium.
2. An alloy according to claim 1, having the following composition by weight:
3. An alloy according to claim 1 having the following composition by weight:
4. An alloy according to claim 1 having the following composition by weight:
5. An alloy according to claim 1 wherein the alloy is subjected to a high temperature thermal treatment to bring into total solution the gama-prime phase, followed by hardening to precipitate the gamma-prime phase, followed by two re-heats.
6. An alloy according to claim 5 wherein the treatment for putting into solution the gamma-prime phase is effected between 1300.degree. C. and 1320.degree. C. for a period of 1 hour to 3 hours, and the two re-heats are effected up to 1100.degree. C. for 3 to 10 hours and at 850.degree. C. for 15 to 25 hours.
Описание
FIELD OF THE INVENTION
The invention relates to monocrystalline alloys with a matrix having a nickel base, without the intentional addition of carbon, or boron or of zirconium.
SUMMARY OF THE PRIOR ART
Such alloys are known for example from FR-A-2 557 598 or from European published application EP-A-0063511.
The object of the invention is to provide a novel group of alloys of the type set forth, suitable for monocrystalline casting, having an elevated solidus temperature (that is in excess of 1325.degree. C.) while at the same time maintaining a practicable thermal treatment spacing between the solidus temperatures and of the gamma-prime solvus phase; Such alloys have, moreover, useful mechanical properties in relation to fatigue strength which render them particularly suitable for use in the aeronautical field, more particularly in the manufacture of the inlet guide nozzle vanes of a turbine.
SUMMARY OF THE INVENTION
This object is achieved in accordance with the invention by alloys having the following composition by weight:
______________________________________ Co 0 to 10% Ta 0 to 6.5% Cr 5 to 7% Al 5 to 7% Mo 1.5 to 2.5% Nb.sup. to 2% W 8.5 to 12.5% Ni balance to 100 ______________________________________
with, in addition the summation of the atomic percentages: 0.005Co+0.036Cr+0.052Mo+0.066W+0.026A1+0.116Nb+0.049Ta less than or equal to 1, these alloys having no titanium.
In order to enable a comparison with other groups of alloys containing, in particular, titanium, the relationship hereinbefore referred to must be applied by applying to the atomic percentage of titanium a multiplying coefficient of 0.078.
BRIEF DESCRIPTION OF THE DRAWINGS
FIG. 1 is a graph showing the effect of the amount of chromium (percentage by weight indicated as the abscissa) on the temperatures (shown as the ordinate) of the liquidus, of the solidus and of the gamma-prime solvus;
FIG. 2 is a similar graph to that of FIG. 1 but is related to the effect of the amount of tantalum;
FIG. 3 illustrates the endurance curve of the Manson Coffin at 900.degree. C. for an alloy in accordance with the invention and two commercial alloys MarM200 Hf with a columnar structure and MarM200 with a monocrystalline structure. The amplitude of the total deformation .DELTA..epsilon.T is indicated as ordinate as a function of the number of cycles to rupture Nf indicated as abscissa;
FIG. 3a illustrates the results of a test similar to those of FIGS. 3 for an alloy in accordance with the invention and another commercial alloy PD21 with a total imposed deformation .DELTA..epsilon.T of 1.2%. The number of cycles to rupture Nf is indicated as ordinate;
FIG. 4 illustrates a similar curve to that of FIG. 3 but applied to a temperature of 1000.degree. C.;
FIG. 5 compares alloys in accordance with the invention with three commercial alloys IN100 with equiaxial structure, Rene 125 with a columnar structure and Mar M200 with a columnar structure, in relation to thermal fatigue, the number of cycles before cracking being indicated as ordinate;
FIGS. 6 and 7 compare respectively at 900.degree. and 1000.degree. C., an alloy in accordance with the invention, an alloy close to the invention and a commercial alloy Mar M 200 with a monocrystalline structure, in relation to the oligocyclic fatigue with imposed deformation. The duration of the life Nf is indicated as abscissa as a function of the total imposed deformation .DELTA..epsilon.T indicated as ordinate.
DESCRIPTION OF THE PREFERRED EMBODIMENT
The introduction of tungsten to an alloy of the kind in question contributes to the stability of the gamma-phrase. It is preferable to maintain the atomic sum Ta+W+Mo+Nb between 5.9 and 6.3 in order to avoid precipitation of a massive primary phase.
The addition of cobalt does not change the temperatures of the liquidus and of the solidus but reduces the temperature of the gamma-prime solvus; cobalt increases the window for return to solution to the gamma-prima phase which facilitates the carrying out of thermal treatment.
The increase in the amount of chromium up to 8% by weight reduces the temperatures of the liquidus, of the solidus and of the gamma-prime solvus (compare FIG. 1) and may give rise to the production of a primary phase.
With regard to the distribution of elements generating gamma-prime phase, the addition of aluminium is preferred to titanium in order to take into account the effect of the reduction of the temperature of the solidus of the alloy since the effect of aluminium is appreciably less than that of titanium. In the relation defined above between the atomic compositions for example, the representative coefficient for titanium of this influence is of the order of three times greater than that of aluminium. For this reason, alloys in accordance with the invention are free of titanium.
The addition of tantalum, the other elements remaining constant, reduces the temperatures of the liquidus and of the solvus, without substantially modifying temperature of the gamma-prime solvus. FIG. 2 has been prepared on the basis of an amount by weight of tungsten of 11%. The substitution of niobium (likewise serving to generate gamma-prime phase) by tantalum is of interest in as far as the solidus temperature increases from 15.degree. to 20.degree. C. However, it is preferable to maintain the amount by weight of tantalum less than or equal to 6.5% in order to avoid substantial fall in the temperature of the solidus. This critical amount of tantalum is a function of the amount of tungsten and thus for an amount by weight of the tungsten of 11, this critical amount must be reduced to 5.5 (compare FIG. 2). The amount of molybdenum, a softening element, is intended to confer an improved strength to the matrix of nickel where it gives rise to a preferential segregation.
By way of example, three alloys N1, B, F in accordance with the invention have been particularly carefully studied. Their composition is given in Table 1, hereinafter, where the amounts are expressed as a percentage by weight and an atomic percentage (between parentheses). The temperatures of the liquidus, solidus and gamma-prime solvus for the alloys in accordance with the invention are set out in Table 2 hereinafter, where they are compared with those which related to commercial monocrystalline alloys Mar M200, CMSX2, SRR99.
Alloys in accordance with the invention, produced in monocrystalline form, are subjected to a sequence of thermal treatments which are appropriate to optimise their properties.
The thermal treatment is initiated by putting into solution gamma-prime precipitates. This is carried out at a temperature lower than the temperature of the solidus between 1300.degree. C. and 1320.degree. C. for a period of one to three hours and for example 1300.degree. C. for one hour for the alloy N1. The cooling is carried out by air hardening, the amount of the gamma-prime precipitates is 0.3.mu.m.
Two further treatments at 1100.degree. C. for three hours to ten hours and at 850.degree. C. for fifteen hours to twenty five hours enable the precipitation of the gamma-prime phase (the amount of gamma-prime precipitates obtained after complete treatment of the alloy N1 is 0.4.mu.m).
The alloy N1 has been tested for oligocyclic fatigue (total imposed deformation) at 900.degree. C. and 1000.degree. C. (FIGS. 3 and 4). It appeared that at 900.degree. C. the alloy had a life expectancy five times greater than that of MARM 200Hf with a known columnar structure in order to provide for good properties during oligocyclic fatigue at high temperature and thermal fatigue. FIG. 3 also illustrates the comparative results for oligocyclic fatigue at 900.degree. C. with a total imposed deformation of 1.2% showing the superiority of the alloy according to the invention N1 with respect to another known alloy having the commercial designation PD21 corresponding to Example 3 of U.S. Pat. No. 4,174,964.
These tests were conducted on test pieces which were treated but in the uncovered condition.
The thermal fatigue tests were effected in the flame zone having a maximum temperature of 1100.degree. C. FIG. 3 brings together the results obtained for the alloys N1, B, F, in accordance with the invention and of other alloys with a columnar structure (MAR M 200 Hf, Rene 125) or equiaxial IN 100 and shows the superiority of alloys in accordance with the invention in which cracks and other faults appear beyond 1000 cycles.
FIGS. 6 and 7 relate to oligocyclic fatigue tests with an effective imposed deformation at 900.degree. and 1000.degree. C. At the two temperatures, MarM200 with a monocrystalline structure served as the reference. The curves give numbers of cycles to rupture as a function of the total imposed deformation. At 900.degree. C. an alloy N5 was also tested which is approaching in composition the group of alloys in accordance with the invention, but not included within the ranges:
______________________________________ Alloy Ni Cr Mo W Ta Al ______________________________________ N5 Base 7.5 2 11 4 6 ______________________________________
The characteristics obtained are inferior to those of the reference N1 belonging to the group of alloys in accordance with the invention.
The series of tests carried out by the applicants illustrate that the alloys of the group in accordance with the invention have improved properties to a significant extent in particular having regard to thermal fatigue and the strength during oligocyclic fatigue, while at the same time having, as has been shown by research, an elevated solidus.
TABLE 1 ______________________________________ B F Nl % % % by wt. % atom % by wt. atom % by wt. atom ______________________________________ Co 0 (0) 5 (5.14) 5 (5.14) Cr 6 (6.85) 6 (6.99) 6 (6.99) Mo 2 (1.24) 2 (1.26) 2 (1.26) Al 6 (13.2) 6 (13.48) 6 (13.48) W 11 (3.55) 11 (3.62) 9 (2.96) Nb 1.8 (1.15) 0 (0) 0 (0) Ta 0 (0) 4 (1.34) 6 (2.01) Ni balance balance balance ______________________________________
TABLE 2 ______________________________________ Temperature Temperature Temperature solvus Alloy liquidus(.degree.C.) solidus(.degree.C.) gamma-prime(.degree.C.) ______________________________________ Nl 1398 1330 1270 B 1408 1350 1282 F 1390 1340 1295 Mar M200 1350 1240 1200 CMS X 2 1375 1325 1265 SRR 99 1370 1305 1260 ______________________________________